Home Tech Library Why Do Thin Film Layers in an AI Chip Film Look Intact but Underperform? TEM Electron Diffraction Reveals Its Crystal Fingerprint

Why Do Thin Film Layers in an AI Chip Film Look Intact but Underperform? TEM Electron Diffraction Reveals Its Crystal Fingerprint

Issued Date:2026/11/26 TEM Electron Diffraction
Issued By:iST

Dr. Bow, Jong-Shing, a renowned expert in materials analysis both domestically and internationally, he jokingly refers to himself as “Uncle Bow”. For over 40 years, he has focused his research on transmission electron microscopy (TEM). He is the author of the book “Practice of Current Transmission Electron Microscopy” and is well-known among beginner TEM learners and engineers.

Over his 40-year career, Dr. Bow has used more than a dozen TEM models and analyzed materials including metals, precision ceramics, semiconductor components, biomedical materials, as well as antiques such as jade and Ru kiln porcelain. During this lecture, Dr. Bao, who has witnessed the evolution of TEM, will share his lifetime of expertise using the most understandable language possible.

AI chips, SiC and GaN devices are becoming ever more precise. TEM images already show that the thin film has formed, yet device performance is still below expectations. TEM images reveal film structure, and EDS and EELS provide elemental or chemical information. But to read a material’s “crystal fingerprint,” you also need another powerful TEM tool, electron diffraction, which gives R&D engineers important clues for tracing process problems.

From advanced AI chip processes to SiC and GaN power semiconductors, the structure of thin films and material interfaces can affect a device’s electrical performance and reliability. When engineers use a TEM to see nanoscale thin films and interfaces, confirming the material’s crystal structure becomes an important topic in R&D and process analysis.

Imagine an R&D scenario: an engineer adjusts the deposition or annealing conditions of a layer of thin film. The TEM image shows that the film has been formed, but the device’s electrical performance does not meet expectations. This raises a question: the TEM image shows that the thickness of the film meets the specification, and EDS composition analysis also shows normal composition. However, no information related to the crystalline phase of the film, correct or not, is available.

Besides thickness and composition of the film, the crystalline phase of the film, including single-crystal, polycrystalline, or amorphous, needs to be known. Is the film an epitaxy on the single crystal substrate? What kind of crystalline phase do elements detected have been formed?

When TEM images and EDS/EELS composition analysis are not enough to answer these questions, electron diffraction offers another way to look into materials. The spot and ring patterns formed after the electron beam passing through the specimen look like a microscopic starry sky. These patterns behave like “crystal fingerprint” of materials, holding clues to its crystal structure, crystal orientation, and arrangement of atoms.

In this episode of Uncle Bow’s Corner” iST Materials Lecture”, Dr. Bow uses cases of materials and thin films to give a short introduction to TEM electron diffraction, a less mentioned fields yet rich in material information. He will help you read this “starry array” and explain what electron diffraction patterns can tell you about materials that TEM images cannot, so engineers can grasp a thin film, crystalline structure as well as morphology.

  • 1. TEM Images Show Material Structure; Electron Diffraction Further Reveals Crystal Information

    Over the past decade, TEM has been widely used in the semiconductor industry to check and characterize nanoscale device structures and thin films. In the semiconductor field, TEM analysis is mainly image-based and supported by EDS analysis. The share of TEM analyses that use electron diffraction patterns (EDPs) is very low.

    However, in materials R&D and process analysis, engineers need to observe not only how a thin film looks, but also to confirm the material’s crystal structure, its orientation, and its relationship with the substrate. The five scenarios below show how electron diffraction can provide analysis clues:

    Table 1: How Does Electron Diffraction Help Engineers? Five Common R&D Scenarios

    R&D ScenarioWhat Engineers May Want to KnowHow Electron Diffraction Helps
    1. The film has formed, but device performance is below expectationsThe film looks complete, but does its internal crystal structure also match the design?Helps identify the crystal type of the analyzed area, such as single-crystal, polycrystalline, or amorphous, as a basis for further analysis.
    2. The elemental composition has been analyzed, and you want to confirm what crystal phase the material formsThe elements in the material are known, but what crystal structure do they form?Provides lattice information that, together with databases and composition analysis, helps identify the likely crystal phase.
    3. A film is deposited on a substrate, and you want to confirm whether it has the expected epitaxial relationshipIs the film’s crystal orientation aligned with the substrate as expected?By comparing the diffraction patterns of the film and the substrate, helps determine the crystal relationship between them.
    4. A good sample and an abnormal sample perform differently, and you need to narrow down the analysis directionDo the two differ in crystal phase or orientation?Compares crystal information between samples to find material differences worth further verification.
    5. After process conditions are adjusted, you want to know what changed in the materialAfter the deposition or annealing conditions change, does the crystal structure change as well?Compares crystal information under different process conditions to guide the next step of process optimization.

    TEMs used to analyze solid inorganic materials typically operate at 200 kV, at which the electron wavelength is 0.0251 Å[1, 2]. This is much smaller than the d-spacings (about 2–3 Å) of many low-index crystal planes of commonly used materials. Diffraction occurs when these high-energy electrons pass through a crystal and the angle between the electron beam and a set of crystal planes satisfies Bragg’s law. EDPs provide crystallographic information about the analyzed specimen down to the sub-ångström scale. Much material information that is hard to extract from TEM images, such as the type of crystal, the crystal orientation, whether a thin film is single-crystal or polycrystalline, and its crystallographic relationship with the substrate, can be readily determined from EDPs.

    Figure 1: Simplified ray-path diagram of the TEM in diffraction mode.
    (Source: iST)

    Figure 1 is a simplified ray diagram of the electron beam in the objective lens region of a TEM. After passing through the crystalline foil, the electrons first form the electron diffraction pattern at the back focal plane of the objective lens, and then, after traveling a further distance, form the image at the first image plane. The EDP is therefore the first product of the interaction between the high-energy electrons and the foil specimen, and it is the basis of all subsequent image analysis. Every TEM image must be taken under a specific diffraction condition in order to give well-defined physical and material information.

    The crystallographic information revealed by an EDP has a spatial resolution better than 1 Å, much higher than that of the images formed afterward. Following the path of the high-energy electrons, the electromagnetic lens behind the objective lens is the intermediate lens (IL). When the IL is weakly excited, it has a long focal length. It takes the EDP at the back focal plane of the objective lens as its “object” and forms a magnified real image of it, which falls exactly on the object plane of the projector lens (PL). The pattern is then magnified once more by the PL and projected onto the TEM fluorescent screen (the image plane of the PL). When an EDP is observed on the screen, the TEM is operating in diffraction mode, which is one of the two basic operating modes of a TEM.

    Figure 2: Typical electron diffraction patterns. (a) Spot SAEDP; (b) nano beam electron diffraction (NBED) pattern of a single crystal; (c) converged beam electron diffraction (CBED) pattern of a single crystal; (d) Kikuchi pattern of a single crystal; (e) FFT pattern of an HRTEM image; (f) ring SAEDP.
    (Source: iST)

    Figure 2 shows four typical single-crystal TEM EDPs (Figures 2(a) to 2(d)): the spot selected area electron diffraction pattern (SAEDP), the NBED pattern, the CBED pattern, and the Kikuchi pattern. Figure 2(e) is the Fourier transform (FFT) pattern of a high-resolution TEM (HRTEM) image, and Figure 2(f) is a ring SAEDP. SAEDPs are taken with a nearly parallel electron beam, and the analyzed area is defined by a selected area diffraction (SAD) aperture at the first image plane. The smallest area that can be analyzed is about 100 nm in diameter.

    NBED, CBED, and Kikuchi patterns are acquired with a focused electron beam. Assuming the probe size is 1 nm where the electron beam strikes the upper surface of the specimen, the diameter of the interaction area at the lower surface is about 3 nm for NBED, which uses a small convergence angle, and about 5 nm for CBED, which uses a larger one. An FFT pattern is not formed directly in the TEM when an electron beam passes through the specimen. Instead, it is obtained by using image processing software to apply a Fourier transform to a square region of an HRTEM image whose side length is a power of two in pixels (2ⁿ pixels). The basic characteristics and functions of the six kinds of diffraction patterns are compared in Table 2.

    Table 2: Comparison of basic characteristics and functions of typical electron diffraction patterns

    Diffraction PatternStatus electron beamMain functionMinimum area analyzedSpecimen
    Spot SAEDPParallel electron beamPhase I. D.
    Measurement of interplanar spacing
    Crystal Orientation Determination
    φ ~ 100 (50) nmSingle crystal
    NBEDPFocused electron beam, small angle.Crystal Orientation Determination
    Strain measurement
    φ ~ 3 nmSingle crystal
    CBEDPFocused electron beam, large angle.Crystal structure
    Strain measurement
    φ ~ 5 nmSingle crystal
    Kikuchi PatternFocused electron beam, small angle.Measurement of interplanar spacing
    Crystal orientation adjustment
    φ ~ 5 nmSingle crystal
    FFT of HRTEM ImagesNonePhase I. D.
    Measurement of interplanar spacing
    2 nm x 2nmSingle crystal
    Ring SAEDPParallel electron beamPhase I. D.
    Measurement of interplanar spacing
    φ ~ 100 (50) nmPoly crystal
  • 2. Spot and Ring Diffraction Patterns Help Identify a Material’s Crystal Type

    The SAEDP is the most commonly used of the EDPs described above, and it contains abundant material information. Take the diffraction patterns in Figure 3 as examples. Figure 3(a) indicates that the analyzed area is a single crystal viewed along a specific crystal orientation. If it is a cubic crystal, the diamond-shaped array of diffraction spots suggests that the orientation is most likely <110>. The ring SAEDP in Figure 3(b) indicates that the analyzed area contains many grains. The corresponding TEM bright-field (BF) image in Figure 3(e) shows the grain structure, a typical polycrystalline structure with well-defined grain boundaries. The SAEDP in Figure 3(c) is an incomplete ring pattern. The diffraction spots of the same radius are not evenly distributed around the ring but are concentrated in a few places, as if the analyzed region contained only a few grains. We call this type of SAEDP a pseudo-ring pattern in this article. However, the corresponding TEM BF image (Figure 3(f)) shows that plenty of small grains are present, but their grain boundaries are blurred.

    A crystal that shows this kind of TEM BF image and SAEDP is called cryptocrystalline. Agate is the typical representative of this type of material. Some high-entropy alloys show similar EDPs[3] as well. The diffuse ring SAEDP in Figure 3(d) indicates that the analyzed region is amorphous.

    Figure 3: SAEDPs and the crystallographic information they contain. (a) Spot SAEDP: single-crystal region; (b) ring SAEDP: polycrystalline region with well-defined grain boundaries; (c) pseudo-ring SAEDP: cryptocrystalline region with blurred grain boundaries; (d) diffuse ring SAEDP: amorphous region; (e) TEM BF image of a typical polycrystal, corresponding to (b); (f) TEM BF image of a typical cryptocrystal, corresponding to (c).
    (Source: iST)

  • 3. Comparing Film and Substrate Diffraction Patterns to Determine Whether There Is an Epitaxial Relationship

    Many semiconductor devices are built on the basic structure of thin films deposited on single-crystal substrates. When a deposited film is itself a single crystal and has a specific crystallographic relationship with the substrate, it is called an epitaxial layer. Unless the magnification reaches the HRTEM level, it is hard to tell from a TEM image whether a deposited film is epitaxial, but a spot SAEDP makes it very easy to judge.

    Figure 4(a) is a TEM BF cross-sectional image of a thin-film/substrate material. It shows a titanium (Ti) thin film deposited on the (0001) plane of a single-crystal 6H-SiC substrate by molecular beam epitaxy (MBE)[4]. Whether the Ti film is epitaxial cannot be judged from this image alone, but comparing the SAEDP of the 6H-SiC substrate (Figure 4(c)) with the SAEDP containing both the substrate and the Ti film (Figure 4(b)) confirms that it is an epitaxial layer. The crystallographic relationship between the Ti film and the 6H-SiC substrate is deduced to be

    (0001)Ti // (0001)6H-SiC
    (-1100)Ti // (-1100)6H-SiC

    The SAEDP in Figure 4(b) contains both the Ti film and the 6H-SiC substrate. Its features show that the Ti film is an epitaxial layer. The pattern also shows that the (0001) and (-1100) plane spacings of Ti are slightly smaller than those of 6H-SiC. Further measurement shows that the Ti (-1100) spacing (0.2555 nm) is 4.0% smaller than the 6H-SiC (-1100) spacing (0.2661 nm). This means that, along the [-1100] direction, a misfit dislocation is expected at the interface about every 6.38 nm.

    Figure 4: High-magnification TEM BF image and SAEDPs of local regions of as-deposited Ti/6H-SiC. (a) TEM image of Ti/6H-SiC; (b) SAEDP of Ti/6H-SiC; (c) SAEDP of the 6H-SiC substrate.
    (Source: iST)

  • 4. Ordinary Images Can Hardly Show GaN Polarity, but Converged Beam Electron Diffraction Provides Clues

    Depositing epitaxial gallium nitride (GaN) layers on sapphire substrates by metal-organic chemical vapor deposition (MOCVD) is the main technology for manufacturing blue light-emitting diodes (LEDs). In general, the atoms in a crystal are arranged symmetrically, so no polarity exists. Under some deposition conditions, however, nitrogen atoms shift from their equilibrium sites in the crystal, which gives the crystal polarity. Neither TEM BF images (Figure 5(a)) nor SAEDPs (Figure 5(b)) can show whether a GaN epitaxial layer has polarity, whereas CBED can, as shown in Figures 5(c) and 5(d).

    In the SAEDP in Figure 5(b), GaN still appears to be a symmetric crystal, but the magnified CBED pattern (Figure 5(d)) clearly shows a difference between the (0002) and (000-2) spots. This asymmetry of the {0002} diffraction spots indicates that this GaN layer has polarity[5, 6].

    Figure 5: TEM BF image of GaN/sapphire, and SAEDP and CBED pattern of the GaN thin film. (a) TEM BF image of GaN/sapphire; (b) SAEDP of the GaN thin film; (c) CBED pattern of the GaN thin film; (d) magnified pattern of the rectangular region in (c).
    (Source: iST)

  • 5. Comparing Diffraction Signals of Precipitates and the Matrix to Understand Their Crystal Relationship

    In many metals, such as stainless steels, aluminum alloys, and nickel-based superalloys, micro- to nano-scale precipitates that strengthen the material form after appropriate thermal annealing. Some of these precipitates have no crystallographic orientation relationship with the matrix, while others have a specific one. The former are called non-coherent precipitates, and the latter are called coherent precipitates.

    The TEM BF image in Figure 6(a) shows two submicron, diamond-shaped precipitates inside a grain of 316 stainless steel. The corresponding SAEDP in Figure 6(b) indicates that these two precipitates are coherent, and that their lattice parameter is three times that of the matrix[7].

    Figure 6: 316 stainless steel. (a) TEM BF image showing two nearly diamond-shaped precipitates; (b) <110> SAEDP, with large spots from the matrix and small spots from the precipitates.
    (Source: iST)

From identifying single crystals and polycrystals to the epitaxial relationship between a film and its single crystal substrate, electron diffraction patterns provide rich material information. But how should we read these star-like diffraction spots and rings?

In the next episode of Uncle Bow’s Corner” iST Materials Lecture”, Dr. Bow will explain how to identify crystals from electron diffraction patterns, work out the viewing direction, and use FFT analysis to measure the d-spacings between lattice planes.

TEM images help engineers to observe material structures, while electron diffraction patterns provide further information such as crystal structure, crystal orientation, and the film-substrate relationship. Combining different analysis methods helps to build a fuller understanding of material properties and offers more clues for material identification and structural failure analysis.

Feel free to contact us: +886-3-5799909 ext. 1065 Ms. Chen │Email: marketing_tw@istgroup.com. We will match you with the most professional technical team to answer your questions!

References:
[1] J. W. Edington, Practical Electron Microscopy in Materials Science, Van Nostrand Reinhold Company, New York (1976).
[2] D. V. Williams and C. B. Carter, Transmission Electron Microscopy, published by Plenum Press, New York, (1996).
[3] Private discussion with Professor Jyh-Wei Lee, Department of Materials Engineering, Ming Chi University of Technology (2024).
[4] J. B. Bow, Dissertation, Arizona State University, (1994).
[5] J. B. Bow, Thesis, Institute of Materials Science and Engineering, National Sun Yat-sen University (1984).
[6] J. Jasinski, Z. Liliental-Weber, Q. S. Paduano, and D. W. Weyburne, “Inversion domains in AlN grown on (0001) sapphire”, Applied Phys. Lett. Vol. 83, No. 14, 2811 (2003).
[7] Fude Liu, Ramon Collazo, Seiji Mita, Zlatko Sitar, Gerd Duscher, and Stephen J. Pennycook, “The mechanism for polarity inversion of GaN via a thin AlN layer: Direct experimental evidence”, Applied Phys. Lett. Vol. 91, 203115 (2007).”

 

Other articles you may be interested in